PROPERTIES AND EMPLOYEMENTS
Il 17NiCrMo6-4 (UNI EN 10084) IS THE NEW DESIGNATION OF 18NiCrMo5 (UNI 7846). IT IS THE MOST COMMON CASE-HARDENING STEEL AND IN ITALY IT IS USED FOR ITS EXCELLENT CHARACTERISTICS THAT MAKE IT SUITABLE FOR SEVERAL APPLICATIONS. IT HAS A MEDIUM-HIGH HARDENABILITY AND A GOOD MACHINABILITY.
AFTER CASE-HARDENING AND HARDENING TREATMENTS, THE SURFACE REACHES AN ELEVATED HARDNESS.
17NiCrMo6-4 IS USED FOR THE PRODUCTION OF MECHANICAL PARTS, WHICH ARE SUBMITTED TO WEAR (GEARS, CAMSHAFTS, BUSHINGS, PINIONS).IS USED FOR THE PRODUCTION OF MECHANICAL PARTS, WHICH ARE SUBMITTED TO WEAR (GEARS, CAMSHAFTS, BUSHINGS, PINIONS).
CORRESPONDENCE TO INTERNATIONAL DESIGNATIONS
QUALITY | EUROPE | GERMANY | FRANCE | SPAIN | G.B. | USA | |
---|---|---|---|---|---|---|---|
EN | DIN | W.n. | AFNOR | UNE | B.S. | AISI/SAE | |
17NiCrMoS6-4 | 17NiCrMoS6-4 | 1.6566 | 18NCD6 | 817M17 | 4317 |
CHEMICAL COMPOSITION % (EN 10084)
STEEL DESIGNATION | CHEMICAL COMPOSITION | |||||||||
---|---|---|---|---|---|---|---|---|---|---|
SYMBOLIC | NUMERIC | C |
Si max |
Mn |
P max |
S | Cr | Mo | Ni | B |
17NiCrMo6-4 | 1,6566 | 0,14 ÷ 0,20 | 0,40 | 0,60 ÷ 0,90 | 0,025 | ≤ 0,035 | 0,80 ÷ 1,10 | 0,15 ÷ 0,25 | 1,20 ÷ 1,50 | - |
17NiCrMoS6-4 | 1,6569 | 0,020 ÷ 0,040 |
CONCENTRATION LIMITS OF THE ELEMENTS THAT ARE NOT INDICATED IN THE TABLE CAN BE DEDUCED IN THE EN 10020 REGULATION. IT CAN BE PROVIDED WITH AN ADDITION OF LEAD 0,12-0,35% OR SULPHUR CONTROLLED UP UNTIL 0,40% FOR AN IMPROVED MACHINABILITY.
MECHANICAL CHARACTERISTICS (UNI 7846)
STEEL QUALITY | BAR'S DIAMETER | TENSILE TESTING |
IMPACT STRENGTH KCU min |
||||
---|---|---|---|---|---|---|---|
UNIFIED TENSILE STRENGTH R |
DEVIATION FROM PROPORTIONALITY Rp 0,2 min |
ELONGATION A min |
|||||
mm | N/mm2 | kgf/mm2 | N/mm2 | kgf/mm2 | % | J | |
18NiCrMo5 |
11 (30) (63) |
1230÷1520 (980÷1270) (830÷1130) |
125÷155 (100÷130) (85÷115) |
980 (735) (635) |
100 (75) (65) |
8 (9) (10) |
30 (32,5) (35) |
JOMINY HARDENABILITY (EN 10084)
STEEL DESIGNATION | RANGE LIMITS | HRC HARDNESS MEASURED FROM THE QUENCHED END OF THE TEST TUBE (MM) | |||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
SYMBOLIC | NUMERIC | 1,5 | 3 | 5 | 7 | 9 | 11 | 13 | 15 | 20 | 25 | 30 | 35 | 40 | |
17NiCrMo6-4+H | 1.6566+H | max | 47 | 47 | 46 | 45 | 43 | 42 | 41 | 39 | 37 | 35 | 34 | 34 | 33 |
17NiCrMoS6-4+H | 1.6569+H | min | 39 | 38 | 36 | 35 | 32 | 30 | 28 | 26 | 24 | 22 | 21 | 20 | 20 |
17NiCrMo6-4+HH | 1.6566+HH | max | 47 | 47 | 46 | 45 | 43 | 42 | 41 | 39 | 37 | 35 | 34 | 34 | 33 |
17NiCrMoS6-4+HH | 1.6569+HH | min | 42 | 41 | 39 | 38 | 36 | 34 | 32 | 30 | 28 | 26 | 25 | 25 | 24 |
17NiCrMo6-4+HL | 1.6566+HL | max | 44 | 44 | 43 | 42 | 39 | 38 | 37 | 35 | 33 | 31 | 30 | 29 | 29 |
17NiCrMoS6-4+HL | 1.6569+HL | min | 39 | 38 | 36 | 35 | 32 | 30 | 28 | 26 | 24 | 22 | 21 | 20 | 20 |
USUALLY AVAILABLE EX STOCK
M.T. COLORATION | QUALITY | HEAT TREATMENT | SURFACE | DIAMETER (mm) |
---|---|---|---|---|
17NiCrMo6-4 | Soft-annealed |
rolled forged turned drawn / peeled h111 |
20-300 330-1200 20-80 |
|
17NiCrMo6-4 high machinability |
Soft-annealed |
rolled peeled |
30-220 22-80 |
|
17NiCrMo6-4+PB | Soft-annealed |
rolled drawn / peeled h111 |
20-200 5-100 |
Download technical sheet |